PGI 1104
Specification1 Revision #1 Effective April 15, 2008 |
|
ASTM
|
PVC 10 |
PVC 20 |
PVC 30 |
PVC 40 |
PVC 50 |
PVC 60 |
||||||
|
Thickness |
D-5199 |
10 +0.5 mil 0.25+.013mm |
20 +1 mil 0.51 + .03 mm |
30 +1.5 mil 0.76 + .04 mm |
40 +2 mil 1.02 + .05 mm |
50 +2.5 mil 1.27 + .06 mm |
60 + 3 mil 1.52 + .08 mm |
|||||
|
Tensile Properties3
Strength at Break
Elongation
Modulus at 100% |
Min (MD & TD) |
24 lbs/in 4.2 kN/m 250% 10 lbs/in 1.8 kN/m |
48 lbs/in 8.4 kN/m 360% 20 lbs/in 3.7 kN/m |
73 lbs/in 12.8 kN/m 380% 30 lbs/in 5.6 kN/m |
97 lbs/in 17.0 kN/m 430% 40 lbs/in 7.0 kN/m |
116 lbs/in 20.3 kN/m 430% 50 lbs/in 8.8 kN/m |
137 lbs/in 24.0 kN/m 450% 60 lbs/in 10.5 kN/m |
|||||
|
Tear Strength |
Min |
2.5 lbs 11 N |
6 lbs 27 N |
8 lbs 35 N |
10 lbs 44 N |
13 lbs 58 N |
15 lbs 67 N |
|||||
|
Dimensional Stability |
Max Chg (MD & TD) |
4% |
4% |
3% |
3% |
3% |
3% |
|||||
|
Low Temperature Impact |
Pass |
-10o F -23o C |
-15o F -26o C |
-20o F -29o C |
-20o F -29o C |
-20o F -29o C |
-20o F -29o C |
|||||
ASTM
|
PVC 10 |
PVC 20 |
PVC 30 |
PVC 40 |
PVC 50 |
PVC 60 |
||||||
|
Specific Gravity |
D-792 Typical |
1.2 g/cc |
1.2 g/cc |
1.2 g/cc |
1.2 g/cc |
1.2 g/cc |
1.2 g/cc |
|||||
|
Water Extraction Percent Loss (max) |
Max Loss |
0.15% |
0.15% |
0.15% |
0.20% |
0.20% |
0.20% |
|||||
|
Average Plasticizer Molecular Weight |
400 |
400 |
400 |
400 |
400 |
400 |
||||||
|
Volatile Loss Percent Loss (max) |
Max Loss |
1.5% |
0.9% |
0.7% |
0.5% |
0.5% |
0.5% |
|||||
|
Soil Burial Break
Strength
Elongation
Modulus at 100% |
Max Chg |
5% 20% 20% |
5% 20% 20% |
5% 20% 20% |
5% 20% 20% |
5% 20% 20% |
5% 20% 20% |
|||||
|
Hydrostatic Resistance |
Min |
42 psi 290 kPa |
68 psi 470 kPa |
100 psi 690 kPa |
120 psi 830 kPa |
150 psi 1030 kPa |
180 psi 1240 kPa |
|||||
|
Seam
Strengths |
ASTM
|
PVC 10 |
PVC 20 |
PVC 30 |
PVC 40 |
PVC 50 |
PVC 60 |
|||||
|
Shear Strength3 |
Min |
20 lbs/in 3.47 kN/m |
38.4 lbs/in 6.7 kN/m |
58.4 lbs/in 10 kN/m |
77.6 lbs/in 14 kN/m |
96 lbs/in 17 kN/m |
116 lbs/in 20kN/m |
|||||
|
Peel Strength3 |
Min |
10 lbs/in 1.8 kN/m |
12.5 lbs/in 2.2 kN/m |
15 lbs/in 2.6 kN/m |
15 lbs/in 2.6 kN/m |
15 lbs/in 2.6 kN/m |
15 lbs/in 2.6 kN/m |
|||||
Notes:1. PGI 1104 replaces PGI 1103 Specification effective 1/1/04.
2. Certified properties are tested
by lot as specified in PGI 1104 Appendix
A or every 18,000 kg (40,000 lbs.).
3. Metric values are converted
from US values and are rounded to the available significant digits.
4. Modifications or further details of test are
described in PGI 1104 Appendix B.
5. Index properties are tested
once per formulation as specified in PGI
1104 Appendix A.
The PGI 1104 Specification was developed with the cooperation of PGI member
companies in order to meet the stringent requirements of today’s geosynthetic
applications. To assure this level of quality, be sure to specify that your PVC
geomembrane is produced and fabricated by a PGI member.
Phone:
217-333-3929 Fax: 217-244-2839 E-mail: pgi-tp@uiuc.edu www.pvcgeomembrane.com